"Galvanized" and "zinc plated" are used interchangeably on drawings and in emails, and the two products are not interchangeable at all. One is a 5–8 µm electroplated film that follows the thread profile exactly. The other is a 45–85 µm metallurgically bonded zinc-iron coating that changes the thread dimensions enough to demand a different nut. The price difference is smaller than most buyers expect; the difference in service life and in assembly behaviour is large.

Two processes, one metal

Zinc plating is electroplating. Bolts are loaded into a barrel, immersed in a zinc electrolyte and given a direct current; zinc deposits on every surface at a controlled rate. The result is a thin, bright, uniform coating — typically 5, 8 or 12 µm, depending on the class called up in ISO 4042 — with a clear or yellow passivation on top. Because the film is thin, a standard 6g bolt thread still runs into a standard 6H nut without modification.

Hot-dip galvanizing is a immersion process. The bolt is cleaned, fluxed and dipped into molten zinc at roughly 445–460 °C. The zinc reacts with the steel and forms zinc-iron alloy layers under an outer layer of nearly pure zinc. The coating is metallurgical, not deposited, and it is thick: ISO 1461 sets minimum values that for fasteners usually land between about 45 and 85 µm, with 50–70 µm the normal commercial range. It is matte grey, slightly rough, and harder than an electroplated film.

Neither process is "better" in the abstract. A zinc-plated bolt indoors will outlive the machine it is fitted to. A zinc-plated bolt on a coastal solar array may show red rust within a couple of years, while a galvanized one is still working after two decades.

PropertyZinc plated (electroplated)Hot-dip galvanized
Typical thickness5–8 µm (up to 12 µm)45–85 µm, usually 50–70 µm
Coating structurePure zinc film, passivatedZinc-iron alloy layers plus zinc
Thread fitStandard 6g / 6H, no allowanceNut must be overtapped or thread cut after coating
Hydrogen embrittlementRisk on 10.9 and 12.9; baking requiredRisk from acid pickling of high-strength steel
Typical exposureIndoor, C1–C2, shelteredOutdoor, C3–C5, coastal and industrial
AppearanceBright, uniform, coloured passivation possibleMatte grey, slight surface variation
Relative costLowHigher per piece, lower per year of life

Thickness and corrosion life

Zinc protects steel sacrificially: the coating corrodes before the base metal, and at a scratch the surrounding zinc keeps protecting the exposed steel. Life is therefore roughly proportional to the mass of zinc present per unit area. An 8 µm electroplated film is around 57 g/m²; a 70 µm hot-dip coating is around 500 g/m². That is the whole argument in one comparison.

It is also why salt-spray hours should be read with care. A plating supplier may quote 96–240 hours to red rust for a passivated zinc film, a galvanizer may quote 500 hours or more for a 70 µm coating, and a zinc-flake supplier will quote a different number again. These tests use different conditions and different failure criteria. For outdoor work, the more useful framework is the corrosivity category of the site — C2 inland sheltered, C3 urban and industrial, C4 coastal, C5 severe marine — combined with the coating mass your specification requires. The category comes from the project, and the required coating mass should be written on the purchase order rather than inferred.

The thread problem and why nuts are overtapped

A hot-dip coating adds thickness on both flanks of the thread, so the pitch diameter grows by roughly twice the coating thickness. A standard nut will not run onto a galvanized bolt; if it is forced, the zinc is sheared off, the thread galls, and the assembly is neither protected nor correctly tensioned. This is the single most common failure we see in galvanized fastener orders, and it is entirely avoidable.

There are two accepted production routes. The first, and by far the most common, is to tap the nut oversize before galvanizing, using a thread tolerance such as 6AZ (or 6AX for larger sizes), which adds roughly 0.4 mm to the pitch diameter in the M12–M24 range. The nut is then galvanized and supplied as a matched set with the bolt, and the pair is test-run by hand before packing. The second route is to cut or roll the thread after galvanizing, leaving bare steel in the thread — acceptable only where the specification allows it and where the exposed thread will be protected.

Centrifuging removes excess zinc from the threads after dipping, but it cannot remove the alloy layer, so it does not restore a standard fit. The practical rule is simple: a galvanized bolt must be ordered with galvanized, overtapped nuts from the same supplier, and the assembly should be checked before it leaves the factory. That is why we supply hex nuts and washers in the same lot as the hex bolts whenever a galvanized order is placed.

Check before you torque. Run one nut onto one bolt by hand from every carton. If it stops before the nut face meets the washer, stop the installation: the thread allowance is wrong, and no amount of wrench force will fix it. A galvanized assembly that galls on site is a coating and tolerance problem, not a tightening problem.

Strength, heat and hydrogen

Electroplating involves acid pickling, and pickling generates hydrogen. In a class 8.8 bolt the risk is modest; in 10.9 and especially 12.9 it is real. Standard practice is to bake electroplated 10.9 within about an hour of plating and hold it at around 200 °C for roughly four hours. Some specifications prohibit electroplating of 12.9 altogether, and that is a defensible position.

Hot-dip galvanizing avoids the electroplating hydrogen route, but it introduces two others. The acid cleaning step before dipping can still charge high-strength steel with hydrogen, which is why some specifications require abrasive blasting instead of acid pickling for 10.9 parts. And the 450 °C dip is a tempering temperature: a 10.9 or 12.9 bolt can lose strength unless the grade and cycle are controlled and the lot is re-tested after coating. Class 8.8 is much less sensitive, which is one reason galvanized 8.8 is the default outdoor structural bolt.

There is a third consideration for preloaded connections: friction. A galvanized faying surface has a lower slip factor than a blast-cleaned one, and the difference must be accounted for in the connection design. If the joint is slip-critical, the surface treatment and the slip factor belong in the specification, not in a note added after fabrication.

Choosing by exposure, then ordering it properly

Start with the environment. Indoors, in a dry plant or under a roof, zinc plating is adequate and cheaper. Outdoors in a temperate inland site, hot-dip galvanizing or zinc flake is the reasonable default. Coastal, marine, industrial or agricultural sites, and any installation expected to last 20 years or more without maintenance, call for hot-dip galvanizing (or a zinc-flake system, which is a separate subject). Where the bolt is 10.9 or 12.9 and outdoors, zinc flake is often the better route than either of the two coatings in this article.

Then write the requirement so it can be checked:

  • Name the standard and the coating mass — ISO 1461 with a minimum coating mass or thickness, or ISO 4042 with the Fe/Zn class. "Galvanized" alone is not a specification.
  • Say how nuts are supplied — "overtapped, galvanized, supplied as a matched set and hand-checked" is a sentence worth adding to every galvanized order.
  • State the strength class and the pre-treatment — especially for 10.9, where acid pickling and baking need a decision before production, not after.
  • Ask for the coating thickness measurement — a magnetic gauge reading on the shank is a five-second check that settles most disputes. Our quality control section describes where those checks sit in the process.
  • Check marking legibility — a thick coating can soften the head stamp. Class and manufacturer identification must still be readable after galvanizing.

The final choice belongs with the engineer of record and the project specification. What we can do is price the two routes honestly, supply the matching nut and washer, and tell you when the coating you have asked for conflicts with the class you have asked for — before the container is loaded, rather than after it is opened on site.