At first glance a class 8.8 and a class 10.9 hex bolt are the same object: the same head, the same thread, often the same carton. The difference is in the steel and in the heat treatment, and it decides how much clamp load the joint can hold, which coatings are safe to apply, and what the assembly costs. Buyers ask us for a one-line answer almost every week. There is no one-line answer, but there is a decision path.

What the numbers on the head actually mean

Both classes are defined in ISO 898-1, and the marking is a two-part code rather than a brand or a trade grade. The figure before the decimal is one hundredth of the nominal tensile strength in MPa: 8 means 800 MPa, 10 means 1000 MPa, 12 means 1200 MPa. The figure after the decimal is ten times the ratio of minimum yield strength to nominal tensile strength: 0.8 for 8.8, 0.9 for 10.9 and 12.9. Multiply the two and you have the minimum yield the lot must meet — 640 MPa for 8.8, 900 MPa for 10.9, 1080 MPa for 12.9.

The standard's tables carry a detail that is often missed. Above M16 the minimum values shift slightly: class 8.8 is tested to 830 MPa tensile and 660 MPa yield, class 10.9 to 1000 and 900, class 12.9 to 1200 and 1080. This is a change in the test method for larger sizes, not a different steel. When you read a mill certificate, match the row to the diameter you bought; a 10.9 certificate quoting 940 MPa is correct for M16 and below, not for M20.

Property classMin. tensileMin. yieldElongationHardnessTypical steel
8.8800 MPa (830 above M16)640 MPa (660)12%250–320 HVMedium-carbon, quenched and tempered
10.91040 MPa (1000 above M16)940 MPa (900)9%320–380 HVCr-Mo alloy, 35CrMo / SCM435 type
12.91220 MPa (1200 above M16)1100 MPa (1080)8%385–435 HVHigher-carbon alloy, quenched and tempered

Where the extra strength goes: preload and fatigue

Tensile strength on a datasheet is not the number the joint feels. A bolted connection works because the bolt is stretched and the plates are clamped; the applied load is carried by the clamp force the bolt keeps, not by the load at which it would break. Class 10.9 lets you put roughly 40% more preload into the same diameter. On a column splice, a tower flange or a machine base, that can mean fewer bolts on the same bolt circle, or a smaller bolt at the same capacity.

The same preload helps fatigue. A bolt tightened close to its working load sees a smaller stress range under repeated loading, so the connection survives more cycles before a crack starts at the first thread. On paper, 10.9 wins both arguments — provided the preload is actually applied.

That is the catch. A 10.9 bolt driven to an 8.8 torque is an expensive 8.8 with a different head stamp. High preload needs a tightening method that controls it: a calibrated torque wrench with a known friction coefficient, or turn-of-nut with a measured angle. It also needs hardened washers and plates that will not crush. On thin sheet, aluminium or a soft gasket the extra clamp load cannot be used, and the stronger bolt simply presses the joint flat.

Rule of thumb, with limits. If the drawing does not name a tightening method, a preload value or a friction coefficient, specifying 10.9 does not buy 40% more joint capacity. It buys a stronger bolt and a higher price. Fix the tightening method first, then choose the class.

When class 8.8 is the better buy

For most balance-of-plant steelwork, solar mounting, machine guards, brackets, cable trays and general assembly, class 8.8 is the correct engineering answer. It is produced in volume in every diameter from M6 to M36, it is available hot-dip galvanized as a routine product, and it tolerates site practice — including a wrench that is not calibrated to the last newton-metre. It is also more forgiving if a bolt is loosened and re-tightened during erection, which happens more often than drawings admit.

Our hex bolt range covers both classes in partial and full thread, and the same lot can be supplied with nuts and washers matched by class. The real price difference between 8.8 and 10.9 is modest per piece — typically 15–30% at the same size and coating — so the decision should follow the joint, not the invoice.

The coating trap that catches 10.9 and 12.9

Two things happen to a high-strength bolt in the coating line. The first is hydrogen. Acid pickling and electroplating generate hydrogen that can enter the steel; in a 10.9 or 12.9 bolt it collects at grain boundaries and the bolt can fail hours or days after installation, under load or even under none. Electroplated 10.9 is therefore normally baked — within about an hour of plating, for roughly four hours at 200 °C — and 12.9 is often not electroplated at all. Many project specifications prohibit it outright, and that prohibition is not conservatism; it is the cheapest risk control available.

The second is heat. Hot-dip galvanizing immerses the bolt in molten zinc at around 450 °C. For a quenched and tempered 10.9 that is a tempering temperature, and hardness and strength can drop unless the steel grade and the dipping cycle are chosen for it and the lot is re-tested afterwards. For 12.9 the risk is greater still. In practice, outdoors and on a 10.9 or 12.9, zinc flake is usually the cleaner coating than galvanizing, and plain oiled is normal where the bolt will be painted or is sheltered.

None of this means galvanized 10.9 is impossible. It means the coating and the class have to be specified together, with a verification step after coating, rather than added one after the other. We quote both and will say which route we recommend for the size and finish on your drawing.

How to write the class on a purchase order

A property class is only enforceable when it is written down with the rest of the part. A purchase order that produces an unambiguous offer normally carries:

  • Standard and thread length — ISO 4014 / 4017 or DIN 931 / 933, with the thread length b stated for bolts over 125 mm.
  • Property class — 8.8 or 10.9, plus the requirement that minimum values are verified per lot by proof load and wedge tensile, not by a single sample at the start of the run.
  • Coating — process, thickness or coating mass, and for 10.9 an explicit baking or coating route.
  • Marking — class plus the manufacturer's identification symbol, legible after coating.
  • Matching nut class — a 10.9 bolt is normally paired with a class 10 nut; a 12.9 bolt with a class 12 nut; galvanized assemblies supplied with overtapped nuts.

Sampling, inspection level and documentation belong in the same document. If certification matters to your project, ask for the heat number on the packing list and a certificate to EN 10204 3.1; our quality control page describes how a lot is checked step by step. For preloaded connections, the assembly — bolt, nut and washer together — is what has to be verified, which is why we supply structural bolting sets as matched kits.

The short version: use 8.8 for most steelwork and take the price and the coating freedom. Move to 10.9 when preload, bolt count, fatigue life or weight is the real constraint, and then spend the effort on the tightening method and the coating route. Your engineer's written specification and the project specification always take priority over a general article, including this one.